Nylon Moisture Absorption Properties
Test Methodology
Test is prepared in reference to ISO 62:2008 Plastics - Determination of water absorption
Preparation
Three specimens are printed in each material:
2 rods 26mm in diameter and 25mm in length printed vertically and horizontally
100mmx100mm plate 2mm thick printed flat
Conditioning
Before testing, the specimens are allowed to cool to room temperature in a sealed container filled with desiccant maintaining a RH of <10% for 24h.
Initial Recording
The specimens are each weighed on a scale, recorded as m1. The lengths of the rods are recorded as l1.
Immersion
The specimens are completely immersed in room temperature tap water for 24 hours, taking care to separate the parts to prevent them from contacting each other.
Second Recording
The specimens are lightly dried with a cloth to remove any surface moisture, and weighed as m2. The lengths of the rods are recorded as l2.
Data
 | m1 (g) | m2 (g) | Δ% |
---|---|---|---|
PA-CF Rod Z | 13.58 | 13.68 | 0.74 |
PA-CF Rod X-Y | 13.87 | 13.95 | 0.58 |
PA-CF Plate | 20.57 | 20.77 | 0.97 |
PA-GF Rod Z | 15.53 | 15.58 | 0.32 |
PA-GF Rod X-Y | 15.52 | 15.59 | 0.45 |
PA-GF Plate | 23.26 | 23.47 | 0.90 |
 | l1 (mm) | l2 (mm) | Δ% |
---|---|---|---|
PA-CF Rod Z | 24.997 | 25.034 | 0.15 |
PA-CF Rod X-Y | 25.059 | 25.081 | 0.09 |
PA-GF Rod Z | 24.608 | 24.634 | 0.11 |
PA-GF Rod X-Y | 24.884 | 24.907 | 0.09 |
Â